S235J0W va S235J2W ikkalasi ham Yevropa standarti (EN 10025-5) ob-havoga chidamli (Corten) po'latlari bo'lib, yaxshilangan atmosfera korroziyaga chidamliligini ta'minlaydi, ko'priklar, jabhalar va avtomobil konstruktsiyalari uchun sirtni himoya qilishni talab qilmaydi. Asosiy farq ularning zarbaga chidamliligini sinovdan o‘tkazishdadir, S235J0W Charpy V-zarbasi 0 daraja zarba energiyasini talab qiladi, S235J2W esa -20 darajada talab qiladi, bu J2W mustahkam va bardoshli tuzilmalar uchun past haroratlarda yaxshi ishlashini ko‘rsatadi.
S235J0W markali mahsulot tahlilining kimyoviy tarkibi
|
C |
Si |
Mn |
Cu |
P |
S |
Cr |
N |
|
0.16 |
0.45 |
0.15-0.70 |
0.20-0.60 |
0.040 |
0.040 |
0.35-0.85 |
0.010 |
S235J2W markali mahsulot tahlilining kimyoviy tarkibi
|
C |
Si |
Mn |
Cu |
P |
S |
Cr |
N |
|
0.16 |
0.45 |
0.15-0.70 |
0.20-0.60 |
0.040 |
0.035 |
0.35-0.85 |
0.010 |
S235J0W sinfining mexanik xususiyatlari
|
Harorat |
-20 |
-10 |
0 |
20 |
|
Teshik ta'siri testi. Min. yutilgan energiya J |
27 |
|
Nominal qalinligi (mm) |
16 gacha |
16 - 40 |
40 - 63 |
63 - 80 |
80 - 100 |
100 - 150 |
|
ReH - Minimal oqish quvvati (MPa) |
235 |
225 |
215 |
215 |
215 |
195 |
|
Nominal qalinligi (mm) |
3 ga |
3 - 100 |
100-150 |
|
Rm -Kuchlanish kuchi (MPa) |
360-510 |
360-510 |
350-500 |
|
Nominal qalinligi (mm) |
1,5<2 dan katta yoki unga teng |
2﹤2,5 dan katta yoki unga teng |
2,5<3 dan katta yoki unga teng |
3<40 dan katta yoki unga teng |
40﹤63 dan katta yoki unga teng |
6﹤100 dan katta yoki unga teng |
100﹤150 dan katta yoki unga teng |
|
A - Minimal cho'zilish Lo=5,65 √ Shunday qilib (%) Uzunlamasına |
19 |
20 |
21 |
26 |
25 |
24 |
22 |
S235J2W sinfining mexanik xususiyatlari
|
Harorat |
-20 |
-10 |
0 |
20 |
|
Teshik ta'siri testi. Min. yutilgan energiya J |
27 |
|
Nominal qalinligi (mm) |
16 gacha |
16 - 40 |
40 - 63 |
63 - 80 |
80 - 100 |
100 - 150 |
|
ReH - Minimal oqish quvvati (MPa) |
235 |
225 |
215 |
215 |
215 |
195 |
|
Nominal qalinligi (mm) |
3 ga |
3 - 100 |
100-150 |
|
Rm -Kuchlanish kuchi (MPa) |
360-510 |
360-510 |
350-500 |
|
Nominal qalinligi (mm) |
1,5<2 dan katta yoki unga teng |
2﹤2,5 dan katta yoki unga teng |
2,5<3 dan katta yoki unga teng |
3<40 dan katta yoki unga teng |
40﹤63 dan katta yoki unga teng |
6﹤100 dan katta yoki unga teng |
100﹤150 dan katta yoki unga teng |
|
A - Minimal cho'zilish Lo=5,65 √ Shunday qilib (%) Uzunlamasına |
19 |
20 |
21 |
26 |
25 |
24 |
22 |
Asosiy xususiyatlar
Turi: past-qotishma, ob-havoga chidamli (Korten) konstruktiv po'lat.
Standart: EN 10025-5.
Oqim kuchi: qalinligi 16 mm gacha bo'lgan minimal 235 MPa.
Kuchlanish kuchi: Odatda 360-510 MPa.
Korroziyaga chidamlilik: himoya zang qatlami (patina) hosil qiladi.
Payvandlash qobiliyati: payvandlangan, perchinlangan yoki murvatli tuzilmalar uchun yaxshi payvandlanish.
"J" belgisi: ta'sirga chidamliligi
J0: 0 gradusda Charpy V-keshigining minimal zarba energiyasi 27J ni bildiradi.
J2: -20 daraja haroratda Charpy V-zarbasining minimal zarba energiyasi 27J ni bildiradi, bu esa sovuqroq sharoitda uni qattiqroq qiladi.
Ilovalar
Ko'priklar, jabhalar, minoralar va me'moriy inshootlar.
Avtomobil va temir yo'l qurilishi.
Konteynerlar va dengiz tuzilmalari (zang hosil qiluvchi{0}}xususiyatlari maqsadga muvofiq).