S420N va S420NL EN 10025-3 standarti bo'yicha normallashtirilgan, nozik konstruktiv po'latlar bo'lib, ular bir xil quvvatni (420 MPa rentabellik) taqdim etadi, lekin past haroratga chidamliligi bilan farqlanadi; S420N -20 daraja haroratda 40 Joul uchun sinovdan o'tgan, o'rtacha sovuq uchun ideal, S420NL esa -50 darajada 27 Joul uchun sinovdan o'tgan yuqori ishlashni taklif qiladi, bu uni arktik yoki dengiz sharoitlariga mos keladi, bu erda haddan tashqari sovuqqa chidamlilik muhim ahamiyatga ega.
EN 10025-3 S420N ning kimyoviy tarkibi
|
Element |
Choynak tahlili (maksimal %) |
Mahsulot tahlili (maksimal %) |
|---|---|---|
|
Uglerod (C) |
0.20 |
0.23 |
|
Kremniy (Si) |
0.60 |
0.70 |
|
Marganets (Mn) |
1.00-1.70 |
1.10-1.80 |
|
Fosfor (P) |
0.025 |
0.035 |
|
Oltingugurt (S) |
0.015 |
0.025 |
|
Azot (N) |
0.025 |
0.030 |
|
Alyuminiy (Al) |
0,020 (daq, jami) |
0,020 (daq, jami) |
|
Niobiy (Nb) |
0.05 |
0.06 |
|
Vanadiy (V) |
0.10 |
0.12 |
|
Titan (Ti) |
0.05 |
0.07 |
|
Xrom (Cr) |
0.30 |
0.35 |
|
Nikel (Ni) |
0.80 |
0.85 |
|
Molibden (Mo) |
0.10 |
0.12 |
EN 10025-3 S420NL ning kimyoviy tarkibi
|
Element |
Choynak tahlili (maksimal %) |
Mahsulot tahlili (maksimal %) |
|---|---|---|
|
Uglerod (C) |
0.20 |
0.22 |
|
Kremniy (Si) |
0.60 |
0.65 |
|
Marganets (Mn) |
1.00-1.70 |
0.95-1.80 |
|
Fosfor (P) |
0.025 |
0.030 |
|
Oltingugurt (S) |
0.020 |
0.025 |
|
Azot (N) |
0.025 |
0.027 |
|
Alyuminiy (Al) |
0,020 (daq, jami) |
0,015 (daq, jami) |
|
Niobiy (Nb) |
0.05 |
0.06 |
|
Vanadiy (V) |
0.20 |
0.22 |
|
Titan (Ti) |
0.05 |
0.06 |
|
Xrom (Cr) |
0.30 |
0.35 |
|
Nikel (Ni) |
0.80 |
0.85 |
|
Molibden (Mo) |
0.10 |
0.12 |
|
Mis (Cu) |
0.55 |
0.60 |
EN 10025-3 S420N ning mexanik xususiyatlari
|
Qalinligi (mm) |
Hosildorlik kuchi (min, MPa) |
Kuchlanish kuchi (MPa) |
Uzayish (min,%) |
Ta'sir energiyasi (min, J @ -20 daraja) |
|---|---|---|---|---|
|
16 dan kam yoki teng |
420 |
520-680 |
19 |
27 |
|
16<> |
400 |
520-680 |
19 |
27 |
|
40<> |
390 |
520-680 |
19 |
27 |
|
63<> |
340 |
520-680 |
19 |
27 |
|
80<> |
290 |
520-680 |
19 |
27 |
|
100<> |
260 |
520-680 |
20 |
27 |
|
150<> |
220 |
500-650 |
20 |
27 |
EN 10025-3 S420NL ning mexanik xususiyatlari
|
Qalinligi (mm) |
Hosildorlik kuchi (min, MPa) |
Kuchlanish kuchi (MPa) |
Uzayish (min,%) |
Ta'sir energiyasi (min, J @ -50 daraja, bo'ylama) |
|---|---|---|---|---|
|
16 dan kam yoki teng |
420 |
520-680 |
19 |
27 |
|
16<> |
400 |
520-680 |
19 |
27 |
|
40<> |
390 |
520-680 |
19 |
27 |
|
63<> |
380 |
520-680 |
19 |
27 |
|
80<> |
360 |
520-680 |
19 |
27 |
|
100<> |
340 |
500-650 |
19 |
27 |
|
150<> |
330 |
500-650 |
19 |
27 |
Asosiy farqlar
S420N: Umumiy qurilish va o'rtacha sovuq muhit uchun javob beradi, -20 daraja ta'sir talablariga javob beradi.
S420NL: sovuqroq iqlim, offshor platformalar va og'ir muhandislik uchun mo'ljallangan, -50 daraja zarba chidamliligini talab qiladi.
O'xshashliklar
Standart: Ikkalasi ham EN 10025-3 ga to'g'ri keladi.
Kuchlilik: Ikkalasi ham 420 MPa minimal oqish quvvatini ta'minlaydi.
Qayta ishlash: ikkalasi ham normallashtirilgan holatda etkazib beriladi.
Tarkibi: Yaxshi payvandlanishi uchun shu kabi past{0}}qotishma, yuqori-kimyoviy kompozitsiyalarni ulashing.
Ilovalar
S420N: Umumiy tuzilmaviy komponentlar, oʻrtacha{1}}vazifa ramkalari.
S420NL: Kranlar, er ko'chirish uskunalari, ko'priklar, kema qurish va juda past haroratli egiluvchanlik zarur bo'lgan dengiz tuzilmalari.