Mahsulot elementlari: soxtalashtirilgan po'lat disk, yotgan bardan kesilgan disk
Material: ASME SB564 N06625 / Incel 625
Diametri: 200 mm
Qalinligi 30 mm
Nace talablari: nice mr0103
Qattiqlik:<35 HRC
625 ta soxta disk yuqori - sifatidan iborat "Asme Sb564" N06625 Matorativ. 200 mm diametri va qalinligi 30 mm bo'lgan qalinligi bilan ushbu disk mustahkamlik va ishonchlilikni ta'minlash uchun joylashtirilgan bardan aniq kesilgan.
Bu MR0103 talablariga javob beradi, uni nordon gaz xizmati va boshqa qiyin talabnomalarda foydalanish uchun ideal qiladi.
Ajralma ekvivalent material va belgi
| 600 ball | En / din 2.4816 | N06600 | 600 |
| 625 | En / din 2.4856 | N06625 | 625 |
| 718 | En / din 2.4668 | N07718 | 718 |
625 Tegishli mahsulotlarni Gnee po'latidan rostlash
| 625 qalbaki halqalar | 625 ta soxta halqalar |
| 625 soxta disk | 625 ta soxta disk |
| 625 soxta halqalar | 625 Shirinlar |
| 625 Kechirad | 625 Shirinlar |
| 625 ta soxta panjara | ASTM B446 AllOY 625 Shirin |
| ASTM B446 AllOY 625 Rasmli halqalar | Asm b446 alyoy 625 Kechiradi |
| 625 ta soxta panjara | 625 ringlar |
| ASTM B446 AllOY 625 halqa | 625 Shirinlar |
| ASTM B446 AllOOY 625 Ruhoniylar uchun | ASTM B446 AllOY 625 Shakllangan barlar |
| AllOY 625 Kechiradi | 625 Fomlar |
| 625 soxta panjara | 625 halqa |
| 625 ringlar |
Noyad SB564 N06625 soxta ring
Biz 625 ta soxta diskori Acme Sb564 Xitoyda n06625 ringni boshqaramiz.
Soxta disk nima?
Forge disk odatdabitta - dona qattiq komponent, xuddi disk kabi, xuddi disk kabi, xuddi disk kabi.
Sanoat uskunalari, klapanlar va boshqa balandlikdagi {{0} yuqori balandlikdagi {{0} yuqori balandlikda foydalanish uchun katta po'latdan yasalgan disklarni yaratish uchun ishlatiladi.
625 disk
625-sonli Nikel - Nikel, uning kuchli kuchi va bosim, oksidlanish va korroziyaga qarshi mashhur.
625 flange, alboy 625, n06625 ekvivalent navli
| Standart | Werkstoff NR. | O'zga emas | Jis | Bs | Gost | Aftidan | Ro'mol | Yoki |
| 625 | 2.4856 | N06625 | NCF 625 | Na 21 | ХН75МБТЮ | NC22DNB4M | Nikr22mo99NB | ЭИ602 |
625 625 Kimyoviy kompozitsiya
| Baho | C | Mn | Si | P | S | Ni | Kri | Fok | Mor | Ko | Aldamoq | Ti | Nb + ta |
| 625 | 0.10 max | 0.50 max | 0.50 max | 0.015 max | 0.015 max | 58.0 min | 20.0 – 23.0 | 5.0 max | 8.0 – 10.0 | 1.0 max | 0.40 max | 0.40 max | 3.15 – 4.15 |
625 Mexanik xususiyatlar
| Zichlik | Erish nuqtasi | Mustahkamlik chegarasi | Hosil berish kuchi (0,2% ofset) | Cho'zish |
| 7.94 g / sm3 | 1385 daraja (2525 f) | Psi - 75,000, MPA - 520 | Psi - 30,000, MPA -205 | 30 % |
We are professional forging disks, forged disks, forged discs, forging discs, steel forging disks, steel forged disks, steel forged/forging discs factory from china
San'atlangan materialning eritilgan usuli - bu ESR + VAR yoki VIM + ESR + VAR
Kvartiralarga ko'ra, bizda 1 tonna, 3 tonna, 6 tonna, 9500 tonna bolg'a va 4500 tonna gidrotovaliligini ochadi.
Biz mijozlarning talabi bo'yicha diskni tashlab, o'rmonni soxtalashtirish uchun oldindan davolash, normalizatsiya qilish, qattiqlashtirish, qattiqlashishni va uni bartaraf etishimiz mumkin.
Folllate - bu po'latdan yasalgan disk, ya'ni biz qila oladigan disk.
Po'lat navlar bilan qoplangan qotishma va uglerod po'latlari:
A182-F1, A182-F9, A182-F21, A182-F22, A182-F92, A694-F42, A694-F46, A694-F46, A694-F46, A694-F48, A694-F48, A694-F48, A694-F50, A694-F70, SA-350 LF2, SA-350 LF3, ASI-350, ASI 410, ASI 4130, ASI 4130, ASISI 4130, ASISI 4130, ASISI 4130, ASISI 4130, ASISI 4130, ASIS 4130, ASISi 8620}, asisi 9840, asisi 4145h, asi 4145h mod, ASI 4330V, ASI 4330V MOD. Aisi 4150, aisi 1020, 42cro4, 34crnimo6, 34crnimao, 16crnimao, 16crnimo4, 16crnimo7, 12cro9-10, 12cro9-10, 18Crmos4, 18crnimo7-6, 17MNCR5, ST52-3, S355J2G3, 50cro4, 39NICMMO3, 20nicRmo2-2
Zanglamaydigan po'lat po'latdan yasalgan ustunlar
A182-F6B, A182-F3B, A182-F310, A182-F316L, A182-F317, A182-F317L, A182-F317L, A182-F317L, A182-F347, A182-F347, ASSI 310S, ASI 310-yillar 316lmod, A182-F321, A182-F347, A182-F348, Nitik 50, Xitik 40, XMRONDON 6, XM-10, F13-8MO, 17-43 va 15-7 / 0-7, f15-7 Mo, 254Smo, Al-6xn, 654smo, A182-F51, A182-F53, A182-F55, A182-F55, A182-F52, A182-F52, A182-F52
Nikel qotishmasi va po'latdan yasalgan super qotish
Nikel 200, Nikel 201, Monel 400, Monel R {{36} {{36} {{36} {{36} {{36} {{36} {{36}, Nimonik 95, Nimonik 80A, Nimonik 105, Nimonic 901, Inconel 600, inconel 601, inconel 617, inconel 625, inconel 686, inconel 690, inconel 693, inconel 718, inconel 725, inconel X-750, incoloy 800, incoloy 800H, incoloy 800HT, Incoloy 825, Incoloy 926, Incoloy 890, Incoloy 925, Indoloy 901, Indoloy 945, Ni-Span-C Alyh 902, Hayu 500, Xaynes, 62, Stellit 36, Kovar qotishmasi, Kovah 4B, Kovab qotishmasi, Koval qotishmasi
No6200, no62002, N06690, N06690, N07618, N07718, N07725, BMI N07725, N07725, N07725, N07725, N07725, N07725, N07725, BU N077550, N08811, N08825, N09925, S66286, N07500, N07500, K93600 bilan
2.4602, 2.4675, 2.4816, 2.4663, 2.4642, 2.4668, 2.4669, 1.4958, 2.4858, 2.4375, 2.4665, 2.4617, 2.4819. 2.4631, 2.4851, 2.4606, 1.4876, 1.4959, 1.4980, 2.4983, 2.4656
TOOK va O'LISH PATELLARNI SAQLASH
AISI 6F7, AISI O2, ASI O2, ASIS D6, AISI A6, AISI A6, H13, H19, H19, H19, H19A, H19A, P20, H19a, P20, P {20+ Ni, p {{{20+ s, s136, 718
SKT6, SKD12, SKD1, SKD2, SKS31, SKS45, SKS43, SKS43, SKD51, SKD5, SKD6, SK72, SK72, Nak80
1.2767, 1.2363, 1.2510, 1.2080, 1.2436, 1.2542, 1.2379, 1.2824, 1.2550, 1.2509, 1.2210, 1.2344, 1.2606, 1.2782, 1.2678, 1.2889, 1.2605, 1.2343, 1.2714, 1.2581, 1.2365, 1.2779, 1.2661, 1.2083, 1.2311, 1.2312, 1.2738, 1.2316
Issiqlikni davolash:
Normallangan / yumshatilgan / qonli
Sirtni davolash:
rasm, plitka, sayqallash, qora oksid, shaffof anti - zang yog'i
Sifatni boshqarish:
UT, MT, RT, PT, kimyoviy kompozitsion test, mexanik mulk test va boshqalar.
Tekshirish:
1, xom ashyo sertifikati (moddiy kimyoviy tarkibi) 2, issiqlik bilan davolash varag'isi to'g'risidagi hisobot
3, O'lchov inspektsiyasi 4, UT sinovi hisoboti
Yetkazib berish holati:
Issiq qal'a + qo'pol ishlov berish (Q / t) + o'girildi